MATERIAL
STAINLESS
Classification Steel Type Density Chemical Composition (%) Mechanical Properties Application Features
0.2% Proof Stress Tensile Strength Elongation Hardness
JIS UNS Number g/cm3 C Si Mn P S Ni Cr Mo Others N/mm2 N/mm2 % HRB(HV)
Austenitic Stainless Steel SUS304 S30400 7.93 ≦0.08 ≦1.00 ≦2.00 ≦0.045 ≦0.030 8.00~10.50 18.00~20.00 - - ≧205 ≧520 ≧40 ≦90 General household utensils, chemical plants, architectural decoration, vehicles
SUS304L S30403 7.93 ≦0.030 ≦1.00 ≦2.00 ≦0.045 ≦0.030 9.00~13.00 18.00~20.00 - - ≧175 ≧480 ≧40 ≦90 Petroleum refining plants, chemical plants, nuclear reactor equipment, paper plants / Intergranular corrosion resistance
SUS304N2 S30452 7.93 ≦0.08 ≦1.00 ≦2.50 ≦0.045 ≦0.030 7.50~10.50 18.00~20.00 - N:0.15~0.30, Nb≦0.15 ≧345 ≧690 ≧35 ≦100 Structural strength members, high-pressure vessels
SUS305 S30500 7.93 ≦0.12 ≦1.00 ≦2.00 ≦0.045 ≦0.030 10.50~13.00 17.00~19.00 - - ≧175 ≧480 ≧40 ≦90 Cold drawn products, expansion-formed parts, spun parts
SUS309S S30908 7.98 ≦0.08 ≦1.00 ≦2.00 ≦0.045 ≦0.030 12.00~15.00 22.00~24.00 - - ≧205 ≧520 ≧40 ≦90 Boiler parts, combustion chamber parts, exhaust systems, gas turbine parts / Heat-resistant steel
SUS310S S31008 7.98 ≦0.08 ≦1.50 ≦2.00 ≦0.045 ≦0.030 19.00~22.00 24.00~26.00 - - ≧205 ≧520 ≧40 ≦90 Boiler parts, combustion chamber parts, exhaust systems, gas turbine parts / Heat-resistant steel, oxidation resistance
SUS312L S31254 8.03 ≦0.020 ≦0.80 ≦1.00 ≦0.030 ≦0.015 17.50~19.50 19.00~21.00 6.00~7.00 N:0.16~0.25, Cu:0.50/1.00 ≧300 ≧650 ≧35 (≦230) Equipment for seawater use, exterior building materials resistant to salt damage, flue gas desulfurization equipment / Resistance to seawater and various acids
SUS316 S31600 7.98 ≦0.08 ≦1.00 ≦2.00 ≦0.045 ≦0.030 10.00~14.00 16.00~18.00 2.00~3.00 - ≧205 ≧520 ≧40 ≦90 Petroleum refining plants, chemical plants, nuclear reactor equipment, paper plants / Corrosion resistance
SUS316L S31603 7.98 ≦0.030 ≦1.00 ≦2.00 ≦0.045 ≦0.030 12.00~15.00 16.00~18.00 2.00~3.00 - ≧175 ≧480 ≧40 ≦90 Petroleum refining plants, chemical plants, nuclear reactor equipment, paper plants / Intergranular corrosion resistance
SUS316LN S31653 7.98 ≦0.030 ≦1.00 ≦2.00 ≦0.045 ≦0.030 10.50~14.50 16.50~18.50 2.00~3.00 N:0.12~0.22 ≧245 ≧550 ≧40 ≦95 Intergranular corrosion resistance, strength members
SUS316J1 - 7.98 ≦0.08 ≦1.00 ≦2.00 ≦0.045 ≦0.030 10.00~14.00 17.00~19.00 1.20~2.75 Cu:1.00~2.50 ≧205 ≧520 ≧40 ≦90 Pitting corrosion resistance, materials for sulfuric acid
SUS316J1L - 7.98 ≦0.030 ≦1.00 ≦2.00 ≦0.045 ≦0.030 12.00~16.00 17.00~19.00 1.20~2.75 Cu:1.00~2.50 ≧175 ≧480 ≧40 ≦90 Intergranular corrosion resistance
SUS317 S31700 7.98 ≦0.08 ≦1.00 ≦2.00 ≦0.045 ≦0.030 11.00~15.00 18.00~20.00 3.00~4.00 - ≧205 ≧520 ≧40 ≦90 Petroleum refining plants, nuclear reactor equipment, dyeing plants, heat exchangers / High-temperature creep resistance
SUS317L S31703 7.98 ≦0.030 ≦1.00 ≦2.00 ≦0.045 ≦0.030 11.00~15.00 18.00~20.00 3.00~4.00 - ≧175 ≧480 ≧40 ≦90 Chemical plants, textile plants / Intergranular corrosion resistance
SUS317LN S31753 7.97 ≦0.030 ≦1.00 ≦2.00 ≦0.045 ≦0.030 11.00~15.00 18.00~20.00 3.00~4.00 N:0.10~0.22 ≧245 ≧550 ≧40 ≦95 Various tanks, containers / High strength, high corrosion resistance
SUS317J2 - 7.98 ≦0.06 ≦1.50 ≦2.00 ≦0.045 ≦0.030 12.00~16.00 23.00~26.00 0.50~1.20 N:0.25~0.40 ≧345 ≧690 ≧40 ≦100 High strength, corrosion resistance
SUS321 S32100 7.93 ≦0.08 ≦1.00 ≦2.00 ≦0.045 ≦0.030 9.00~13.00 17.00~19.00 - Ti:≧5*C% ≧205 ≧520 ≧40 ≦90 Welded structures for high temperatures, jet engine parts, pressure cookers, chemical plants
SUS347 S34700 7.98 ≦0.08 ≦1.00 ≦2.00 ≦0.045 ≦0.030 9.00~13.00 17.00~19.00 - Nb≧10*C% ≧205 ≧520 ≧40 ≦90 Welded structures for high temperatures, chemical plants, energy-related plants
SUS836L S32053 8.06 ≦0.030 ≦1.00 ≦2.00 ≦0.045 ≦0.030 24.00~26.00 19.00~24.00 5.00~7.00 N≦0.25 ≧275 ≧640 ≧40 (≦230) Valves for paper industry, food plants, salt plants, seawater heat exchangers / Pitting corrosion resistance
SUS890L N08904 8.05 ≦0.020 ≦1.00 ≦2.00 ≦0.045 ≦0.030 23.00~28.00 19.00~23.00 4.00~5.00 Cu:1.00~2.00 ≧215 ≧490 ≧35 (≦200) Chemical plants, various equipment for seawater use / Acid resistance, seawater resistance
Ferritic Stainless Steel SUS405 S40500 7.75 ≦0.08 ≦1.00 ≦1.00 ≦0.040 ≦0.030 - 11.50~14.50 - Al:0.10~0.30 ≧175 ≧410 ≧20 (≦200) Mechanical structural parts, food plants, chemical plants, quenched parts, clad materials
SUS410L - 7.75 ≦0.030 ≦1.00 ≦1.00 ≦0.040 ≦0.030 - 11.00~13.50 - - ≧195 ≧360 ≧22 (≦200) Automobile exhaust systems, boiler combustion chambers, burners / Workability, high-temperature oxidation resistance
SUS430 S43000 7.70 ≦0.12 ≦0.75 ≦1.00 ≦0.040 ≦0.030 - 16.00~18.00 - - ≧205 ≧450 ≧22 (≦200) General household utensils, commercial kitchen equipment, distillation apparatus
SUS434 S43400 7.70 ≦0.12 ≦1.00 ≦1.00 ≦0.040 ≦0.030 - 16.00~18.00 0.75~1.25 - ≧205 ≧450 ≧22 (≦200) Automotive moldings, fasteners, road maintenance materials / Salt resistance
SUS444 S44400 7.75 ≦0.025 ≦1.00 ≦1.00 ≦0.040 ≦0.030 - 17.00~20.00 1.75~2.50 8x(C%+N%)≦Ti+Nb+Zr≦0.80 ≧245 ≧410 ≧20 (≦230) Water heater boilers, electric water heaters / Corrosion resistance, stress corrosion cracking resistance
Martensitic Stainless Steel SUS410 S41000 7.75 ≦0.15 ≦1.00 ≦1.00 ≦0.040 ≦0.030 - 11.50~13.50 - - ≧205 ≧440 ≧20 (≦210) For cutlery, mechanical structural members, general household utensils
SUS410S S41008 7.75 ≦0.08 ≦1.00 ≦1.00 ≦0.040 ≦0.030 - 11.50~13.50 - - ≧205 ≧410 ≧20 (≦200) For cutlery, mechanical structural members, general household utensils / Corrosion resistance, formability
SUS420J1 S42000 7.75 0.16~0.25 ≦1.00 ≦1.00 ≦0.040 ≦0.030 - 12.00~14.00 - - ≧225 ≧520 ≧18 (≦234) Turbine blades / Hardenability by quenching
SUS420J2 S42000 7.75 0.26~0.40 ≦1.00 ≦1.00 ≦0.040 ≦0.030 - 12.00~14.00 - - ≧225 ≧540 ≧18 (≦247) Knives, nozzles, valves, rulers / Hardenability by quenching
Austenitic-Ferritic Stainless Steel SUS327L1 S32750 7.80 ≦0.030 ≦0.80 ≦1.20 ≦0.035 ≦0.020 6.00~8.00 24.00~26.00 3.00~5.00 N:0.24~0.32, Cu:≦0.50 ≧550 ≧795 ≧15 HBW≦310 Seawater pumps, seawater desalination plants, heat exchangers / Pitting corrosion resistance, crevice corrosion resistance
- S32760 7.80 ≦0.030 ≦1.00 ≦1.00 ≦0.030 ≦0.010 6.0~8.0 24.0~26.0 3.0~4.0 N:0.20~0.30, Cu:0.50~1.00, W:0.50~1.00 ≧550 ≧750 ≧25 HBW≦310 Seawater desalination plants, chemical plants, seawater pumps / Pitting corrosion resistance
SUS329J3L S31803 7.80 ≦0.030 ≦1.00 ≦2.00 ≦0.040 ≦0.030 4.50~6.50 21.00~24.00 2.50~3.50 N:0.08~0.20, Cu, W ≧450 ≧620 ≧18 (≦320) Oil well pipe, chemical tankers, chemical equipment / Resistance to hydrogen sulfide and chloride environments
- S32205 7.80 ≦0.030 ≦1.00 ≦2.00 ≦0.040 ≦0.030 4.50~6.50 21.00~24.00 2.50~3.50 N:0.14~0.20, ≧450 ≧620 ≧18 (≦301) Seawater pumps, seawater desalination plants, paper plants / Pitting corrosion resistance, crevice corrosion resistance NAS 74N
SUS329J4L S31260 7.80 ≦0.030 ≦1.00 ≦1.50 ≦0.040 ≦0.030 5.50~7.50 24.00~26.00 2.50~3.50 N:0.08~0.30, Cu, W ≧450 ≧620 ≧18 (≦320) Seawater heat exchangers, salt plants / Resistance to high-concentration chlorides, SCC resistance
- S39274 7.80 ≦0.030 ≦0.80 ≦1.00 ≦0.030 ≦0.020 6.0~8.0 24.0~26.0 2.5~3.5 N:0.24~0.32, Cu:0.20~0.80, W:1.50~2.50 - - - - Undersea operation pipe, seawater heat exchanger pipe / Pitting corrosion resistance, seawater resistance, crevice corrosion resistance
- S32808 7.80 ≦0.030 ≦0.50 ≦1.10 ≦0.030 ≦0.010 7.0~8.2 27.0~27.9 0.80~1.20 N:0.30~0.40, W:2.10~2.50 - - - - Urea reactor piping / Urea corrosion resistance, stress corrosion cracking resistance

*Please note that each manufacturer may have their own unique materials (steel types) for each shape, so please consult with our sales representatives.
*The data listed on this page are representative values independently researched by our company, based on JIS standards and manufacturer published values, among other references.These are for reference only and we do not guarantee the accuracy, completeness, or suitability of the values.Please be sure to verify the information yourself before use.